Application-first concrete fibre engineering[email protected] · WhatsApp +86 159 6543 3989
Technical Article

Why Does UHPC Crack at Early Age? Autogenous Shrinkage, Temperature, Restraint and Curing

November 9, 2026

Early-age UHPC cracking is rarely determined by one “shrinkage value”. Volume changes develop during the plastic stage, early hydration and moisture loss, while temperature changes act at the same time. When moulds, reinforcement, connectors, adjacent materials or component geometry restrain that movement, strain can become tensile stress and a crack may form. The correct approach is to separate mechanisms by time and boundary condition, control moisture loss, temperature and restraint, and treat fibre as a controlled trial variable rather than a universal cure.

Why does early-age UHPC risk require separate management?

UHPC commonly has a low water-to-binder ratio and a high binder content. As early strength develops, internal humidity, chemical reactions and temperature also change quickly. FHWA structural design guidance for UHPC separates drying and autogenous shrinkage and notes that autogenous shrinkage is proportionally greater than in conventional concrete and occurs mainly during early strength development.

“Strength has developed” does not mean “cracking risk has passed”. Elastic modulus, tensile capacity and the ability to creep or relax stress are changing during the same period. Free shrinkage measured on a specimen is not the same as cracking risk in a component. The latter also depends on the degree of restraint and whether stress develops faster than the material can resist it at that age.

How should plastic, autogenous, drying and thermal effects be separated?

The purpose of classification is not to assign one label to every crack. It is to decide what to measure, what to change and when to set a hold point.

Mechanism or action Typical period and condition What to check on site Priority control and measurement Conclusion that cannot be drawn directly
Plastic-stage moisture loss and volume change Before and around setting; surface evaporation, wind, temperature or a large exposed area Time of cracking, surface skinning, interval from casting to covering, environmental record Reduce exposure, cover promptly or use an approved curing measure; record surface and ambient conditions Every surface crack is autogenous shrinkage
Autogenous shrinkage During early hydration and falling internal relative humidity; can occur under sealed external conditions Water-to-binder ratio, binder system, internal temperature and humidity, sealing and free movement Begin sealed or free-shrinkage measurement as early as the method requires and align it with strength and temperature histories A later-age drying test captures the early autogenous period
Drying shrinkage Associated with external moisture exchange; influenced by exposed area, environment and curing Demoulding time, end of sealing, humidity, thickness and exposed faces Define curing and exposure boundaries; record moisture condition and length change Every drying effect is autogenous shrinkage
Hydration heat and temperature gradient Rise, peak and cooling after casting; greater concern around thickness changes Internal and surface temperatures, mould and ambient temperatures, insulation and demoulding time Place temperature sensors and control material, mould, insulation and cooling conditions Ambient temperature represents the component core
Restraint Whenever moulds, reinforcement, inserts, substrate, existing concrete or geometry restrict free movement Contact and fixing, ends, openings, corners, thickness changes and demoulding sequence Connect free strain to cracking risk through a restrained method or component-relevant observation Low free shrinkage guarantees a crack-free component

One crack may involve several actions. A surface can lose moisture before covering while internal temperature rises and an insert restrains local movement. Only a retained timeline can show which early abnormality coincided with which boundary change.

Why does restraint turn volume change into cracking risk?

A free-shrinkage specimen asks how much the material tends to shorten. A restrained test or real component asks what happens when that shortening is limited. They are not the same metric. Research on early-age PP-fibre UHPC behaviour evaluates free autogenous shrinkage, restrained stress, tensile creep and cracking potential separately, showing why one free-shrinkage number cannot determine restrained cracking.

Sources of restraint in components include:

  • mould friction, fixed ends and asymmetric release;
  • reinforcement, connectors, lifting points, inserts or incompatible movement between materials;
  • thin wings, openings, sharp corners, thickness changes and local strain concentration in slender components;
  • staged casting, repair or connection zones where old and new materials move differently;
  • humidity or temperature gradients between the surface and core.

A plant record should therefore say more than “a crack appeared”. It should record the first observation time, location, direction and length or width method, then relate those observations to the temperature peak, curing transition, mould release, demoulding and handling.

Why must curing begin as early as the process requires?

Early-age risk can develop before the surface appears hard. At minimum, the curing plan should define the permitted interval from casting to first cover, whether the surface is sealed, the in-mould stage, temperature and humidity boundaries, any heating or insulation regime, demoulding conditions, continued curing after demoulding and who approves a deviation.

Research on plastic and early-age UHPC shrinkage shows that water-to-binder ratio, silica fume, sealed or unsealed conditions, and internal temperature and humidity can affect early volume change. It supports measurement around the actual material and boundaries, but it does not prescribe one curing duration for every plant.

For complex decorative components or components with a large surface area, include edges, back faces, openings and surface-finishing operations. If an appearance process delays covering, that exposure must be a trial variable and deviation record; it cannot be ignored after an unfavourable result.

Can PP fibre solve early-age cracking in UHPC?

PP fibre can be one controlled variable in a trial plan, but it cannot replace moisture-loss, temperature, restraint and curing controls. Published experiments show that the response depends on fibre characteristics, dosage, mix, degree of restraint, method and time window. Feng et al. report dosage- and restraint-dependent early-age behaviour; more PP fibre did not produce unlimited benefit.

Modified PP 12 is a transparent, fine, round modified PP monofilament with no physical embossing, a standard length of 12 mm and an equivalent diameter of 0.20 mm. Its TDS gives 9–15 kg/m³, by mass of fibre per cubic metre of concrete, as a starting trial range. It is not a universal design dosage or a guaranteed shrinkage or crack-control value. Single-fibre tensile strength, elongation at break and elastic modulus likewise cannot predict free shrinkage, restrained stress or component cracking.

Use a control mix without the trial variable. Keep raw-material batches, batch size, mixing, casting, curing and test conditions comparable, then observe workability, fibre distribution, free movement, restrained response and the component surface. If curing, material batch or charging method changes at the same time, the difference cannot be attributed to fibre alone.

Review controlled product identity on the Modified PP 12 product page and use the Laboratory page to plan the route from material checks to component verification.

How should hold points run from diagnosis to release?

The investigation can be divided into four stages, each with a record and a condition for proceeding.

Stage Required record Suggested hold point Example decision
Define the baseline Current mix, raw-material batches, mixer, environment, mould, geometry and existing crack timeline Are the control data complete and repeatable? Repeat the baseline before comparing fibre if the data are inadequate
Measure mechanisms Early free movement, internal and surface temperatures, environment, covering and demoulding times Did measurement begin early enough and are boundaries clear? Do not assign cause if time zero or temperature history is missing
Restrained and component-relevant verification Restraint method, inserts, reinforcement, mould condition, crack map, workability and dispersion Do specimens represent the critical restraint and geometry? A free specimen alone cannot release the component
Production scale-up Actual batch, charging, mixing, casting, curing, demoulding, handling and deviations Were acceptance limits and signatories agreed in advance? Retest or accept conditionally if conditions change or a deviation exceeds the limit

Connect this route to the project conditions on the UHPC Solution; do not transfer a literature result directly to the production line.

Early-age cracking investigation and trial checklist

  • [ ] State the decision for this round: crack mechanism, process deviation or the effect of one control measure.
  • [ ] Record exact times for casting, covering, temperature peak, mould release, demoulding, handling and first crack observation.
  • [ ] Mark crack location, direction and measurement method on the same drawing as openings, corners, inserts and thickness changes.
  • [ ] Record plastic-stage exposure, autogenous-shrinkage measurement, external drying and temperature history separately.
  • [ ] Retain both free-movement and restrained or component-relevant observations.
  • [ ] Define restraint from moulds, reinforcement, connectors, substrate or adjacent materials.
  • [ ] Fix the control conditions, change only the planned variable and record every deviation.
  • [ ] In a fibre trial, check workability, fibre balls, distribution, casting and surface condition together.
  • [ ] Agree acceptance limits, measurement times, retest conditions and final approval authority in advance.
  • [ ] Issue a condition-specific decision only after material and component evidence meet project requirements.

Can say / cannot say

Can say Cannot say
Early-age UHPC cracking risk requires consideration of autogenous shrinkage, drying or plastic moisture loss, temperature and restraint UHPC cracking has one cause
Curing, environment, geometry, moulds and inserts can change component risk Adequate later-age compressive strength guarantees no early-age cracking
PP fibre may be assessed as a controlled variable; response depends on the actual system and restraint Adding PP fibre guarantees crack prevention, or more fibre is always better
The TDS 9–15 kg/m³ value is a starting trial range 9–15 kg/m³ is a universal design dosage, shrinkage guarantee or steel-fibre replacement ratio
The project should predefine measurement, limits and approving parties Generic literature can provide a product- or component-specific performance result

Frequently asked questions

1. Is every early-age UHPC crack caused by autogenous shrinkage?

No. Autogenous shrinkage is important, but plastic-stage moisture loss, later drying, internal heating and cooling, temperature gradients, and restraint from moulds or inserts may also contribute. Use timing, location and boundary records to diagnose the case.

2. Does lower free shrinkage mean that the component will not crack?

No. Free shrinkage describes movement under low restraint. Component cracking also depends on restraint, tensile capacity at that age, stress relaxation and geometric concentration. Restrained or component-relevant evidence is still required.

3. When should early-age movement and temperature recording begin?

Begin at the time defined by the project method and as close to casting as the method requires. State time zero, sealed or exposed boundaries and sensor locations. Starting too late may miss major early changes.

4. Can the Modified PP 12 range of 9–15 kg/m³ be used directly for every UHPC?

No. It is the TDS starting trial range. The target component, mix, process and responsible party must define trial points and acceptance limits; it is not a universal design dosage.

5. Can compressive-strength testing alone verify a crack-control plan?

No. It cannot replace early free-movement, temperature, restrained response, crack observation, workability, dispersion and component-relevant checks. Select tests around the predefined risk and decision question.

Next step: bring the timeline and restraint into a controlled trial

If the project has early-age cracking, or if curing, process and Modified PP 12 variables are to be compared, assemble the component drawing, mix, mixing and casting records, temperatures, environment, curing and crack timeline. Then submit a UHPC plant-trial enquiry. The enquiry supports verification planning; it is not structural design or performance approval.

Public sources and evidence boundaries

Accessed 9 November 2026.

  1. FHWA, Structural Design with Ultra-High Performance Concrete, FHWA-HRT-23-077. https://highways.fhwa.dot.gov/sites/fhwa.dot.gov/files/FHWA-HRT-23-077.pdf — distinguishes autogenous and drying shrinkage and supports early-age risk management; not a project limit.
  2. FHWA, Ultra-High Performance Concrete: A State-of-the-Art Report for the Bridge Community, Chapter 3, FHWA-HRT-13-060. https://www.fhwa.dot.gov/publications/research/infrastructure/structures/hpc/13060/003.cfm — supports early measurement and general UHPC behaviour; not component approval.
  3. Shen et al., “Early-age autogenous shrinkage, tensile creep, and restrained cracking behavior of ultra-high-performance concrete incorporating polypropylene fibers”, Cement and Concrete Composites 138 (2023) 104948. https://doi.org/10.1016/j.cemconcomp.2023.104948 — distinguishes free shrinkage, restrained stress, tensile creep and cracking potential; results are not transferable without project verification.
  4. Feng et al., “Effect of polypropylene fiber on early-age properties and stress relaxation of ultra-high-performance concrete under different degrees of restraint”, Journal of Building Engineering 68 (2023) 106035. https://doi.org/10.1016/j.jobe.2023.106035 — supports dosage- and restraint-dependent behaviour; not Modified PP 12 validation.
  5. “Plastic and early-age shrinkage of ultra-high performance concrete (UHPC)”, Case Studies in Construction Materials 16 (2022) e00948. https://doi.org/10.1016/j.cscm.2022.e00948 — supports attention to water-to-binder ratio, sealing, temperature, humidity and early volume change; not a universal curing regime.